The fired glaze exhibits a network of fine cracks. These may be plainly visible after firing or may need enhancement with ink. Crazing may also appear after a period of time or after ware has been exposed to thermal shock. Fired strength (an thus functional ware quality) are directly related to crazing since ware strength is enhanced by having the glaze under slight compression whereas it is severely reduced (up to four times less) when the glaze is under tension. If the underlying clay matrix is porous and soaks up water then safety could be a concern with crazed ware since the cracks could be wide enough to provide a friendly breeding ground for colonies of bacteria. Containers used to store food are a special concern since a small colony in a crack can become a large culture in the food. If you have any doubt whether this is an important issue ask a commercial food service inspector about the subject.
If pieces must survive considerable thermal shock during use, then both ware and glaze need to have a low and linear thermal expansion curve and they must be compatible. This is difficult to achieve in low fire ware because little mullite or other low-expansion silicate minerals develop during firing. If your low fire body contains significant talc, reduce or eliminate it (also adjust glazes to have a lower expansion so they continue to fit the body). If your high fire body develops non-linear expanding cristobalite during firing, find a way to reduce this.
High temperature firing is by far the best for the production of low-expansion ware. Many more minerals are available for both body and glaze mixes and higher temperatures produce low-expansion silicates and aluminates that give tough glaze and body matrixes capable of withstanding forces that might otherwise cause crazing.
If ceramic ware is porous it can soak up water that causes the ware to expand, thereby putting tension on the glaze and crazing it.
Fired ceramic expands and contracts as it is heated. If the fired glaze has a significantly higher co-efficient of expansion than the body then no amount of careful firing or thin glazing will avoid the inevitable crazing. This is by far the most common cause of crazing and solution strategies are case studies of applying ceramic calculations to solve problems. If even only one piece crazes it is often a sign that all the other ware in that kiln will eventually craze. Such glazes usually need drastic changes since crazing is a visible manifestation of a fit problem that has already greatly reduced ware strength. Lower temperatures are far more sensitive in this respect in that there is a much narrower range within which a glaze and body will be compatible.
To improve glaze fit adjust the clay body to give it higher expansion and thereby the greater contraction that compresses glazes to prevent crazing (i.e. increase flint for high temperature bodies, talc at low fire). You can also adjust the glaze to reduce its expansion. There are many ways to do this. For example, if the glaze is melting well and it is not a matte, try increasing the silica. Or try introducing boron at the expense of some of the flux since B2O3 contributes to both glass development and melting. You can also introduce fluxing oxides of lower expansion at the expense of those with higher expansion in such a way that the fired properties are not changed too much; for example try adding CaO, MgO, or ZnO at the expense of Na2O and K2O (crazing is most serious with sodium and potassium glazes, to demonstrate mix nepheline syenite and water and apply as a glaze and fire at high temperature). If your glaze is opaque try using more low-expansion zirconium opacifier or use it instead of tin or titanium. Zirconium opacifiers are also useful in transparent glazes; they have a threshold amount under which they do not normally opacify. Thus it might be possible to add as much as 5% to make the glaze both more durable and reduce its expansion.
If the body expansion is too low (i.e. ovenware and flameware bodies) it can be very difficult to fit a glaze that has the desired visual characteristics. Lithium can dramatically reduce the thermal expansion of glazes, but its use requires a lot of testing since its contribution is not linear and it introduces other dynamics that must be considered.
Generally increased additions of iron and copper oxide to a glaze will reduce crazing (if they are present in adequate amounts; beyond 1 or 2 percent). Cobalt could have a moderate lowering effect, but since so little is typically used in glazes it will not be significant.
Underfired bodies may contain uncombined alkali or alkaline earths than can react with water and swell the body. You can test this by putting a glazed sample in a pressure cooker for several hours.
Normally a glaze/body combination with compatible expansion characteristics will withstand considerable firing and usage abuse without displaying signs of crazing. However, in some cases, a glaze that otherwise 'fits' will craze if applied very thick.
Also, if the kiln is cooled very quickly or unevenly, especially if ware is thicker, the severe stresses can produce crazing. However remember that a glaze's ability to withstand normal or even quick kiln cooling is an indicator of its ability to resist crazing in normal use.
If you are cooling your kiln very slowly to prevent ware from crazing it is likely the glaze does not fit. While it may be true that slower firing seems to solve the problem, time will bring out the crazing that the kiln did not. In fact if you must slow cool to prevent crazing it is a virtual certainty that your glaze needs to have its thermal expansion reduced.
Special Note: The book "The Magic of Fire II" deals with this subject in great detail. Solving crazing problems while retaining the visual character of a glaze is a classic problem for the application of ceramic chemistry calculations.
Box 432, Cornwall, PE, C0A 1H0 Canada Phone Phone: (406) 662-0136 |