Digitalfire Recipe Database

Logged in as Level 2 access: Logout


Ravenscrag Slip plus 10% dolomite

CodeGR10-F
Modification Date2011-08-02 17:27:51
Member of GroupRV10
DescriptionPlainsman Cone 10R Ravenscrag Slip Glaze

Recipe

MaterialAmountUnits+/-*Stat
Ravenscrag Slip90.00kg  
Dolomite10.00kg  
Red Iron Oxide1.50kg  
 101.50  

Firing Schedule

Rate (C)Temp (C)Hold (Min)Step
~10 pilots10001
5055002
10098003
50130004
01300305
Freefall306



Feedback, Suggestions

Your email address

Subject

Your Name

Message


Copyright 2003, 2008 http://digitalfire.com, All Rights Reserved
Get a free INSIGHT software trial

INSIGHT is ceramic chemistry
calculation software that runs on
Windows, Mac and Linux and talks
to this web site. ()