Digitalfire Recipe Database

Logged in as Level 2 access: Logout


Ravenscrag Slip plus 10 Whiting

CodeGR10-B
Modification Date2011-08-02 17:26:02
Member of GroupRV10
DescriptionCone 10 Reduction Glaze

Recipe

MaterialAmountUnits+/-*Stat
Ravenscrag Slip90.00kg  
Whiting10.00kg  
 100.00  

Firing Schedule

Rate (C)Temp (C)Hold (Min)Step
~10 pilots10001
5055002
10098003
50130004
01300305
Freefall306