Recipe

MaterialAmountUnits+/-*Stat
Ravenscrag Slip70.00kg  
Dolomite15.00kg  
Ferro Frit 313415.00kg  
Copper Oxide Black2.00kg  
Cobalt Carbonate0.50kg  
Rutile Ceramic5.00kg  
 107.50  

Firing Schedule

Rate (C)Temp (C)Hold (Min)Step
551041201
16748202
8359303
16794504
601185205
278103506
8381607