Recipe

MaterialAmountUnits+/-*Stat
Ravenscrag Slip70.00kg  
Light Magnesium Carbonate2.00kg  
Dolomite13.00kg  
Ferro Frit 313415.00kg  
Rutile5.00kg  
Cobalt Oxide2.00kg  
Copper Oxide Black1.00kg  
 108.00  

Firing Schedule

Rate (C)Temp (C)Hold (Min)Step
551041201
16748202
8359303
16794504
601185205
278103506
8381607