Ravenscrag Recipe D: Black Glossy Cone 6| Code | GR6-D |
| Modification Date | 2011-08-02 17:50:04 |
| Member of Group | RV6 |
| Description | Plainsman Cone 6 Ravenscrag Slip Glaze |
Recipe| Material | Amount | Units | +/- | *Stat |
| Ravenscrag Slip | 80.00 | kg | | |
| Ferro Frit 3134 | 20.00 | kg | | |
| Iron Oxide Red | 13.00 | kg | | |
| Cobalt Oxide | 0.50 | kg | | |
| Chrome Oxide | 0.50 | kg | | |
| | 114.00 | |
Firing Schedule
| Rate (C) | Temp (C) | Hold (Min) | Step | | 55 | 104 | 120 | 1 | | 167 | 482 | 0 | 2 | | 83 | 593 | 0 | 3 | | 167 | 945 | 0 | 4 | | 60 | 1185 | 20 | 5 | | 278 | 1035 | 0 | 6 | | 83 | 816 | 0 | 7 |
|