Gizmo Ball Clay
| L5M - % < 0.5 microns |
20% |
| WABS - Water absorption |
Cone 9: 8.0% |
| FSHR - Firing Shrinkage |
Cone 9: 4.0% |
| DSHR - Drying Shrinkage |
6.4% |
| MOR5 - Dry M.O.R. (50% Silica) |
170 psi |
Out Bound Links
XML for Import into INSIGHT
<?xml version="1.0" encoding="UTF-8"?>
<material name="Gizmo Ball Clay" descrip="" searchkey="" loi="0.00" casnumber="70694-09-6">
<oxides>
<oxide symbol="CaO" name="Calcium Oxide, Calcia" status="" percent="0.500" tolerance=""/>
<oxide symbol="MgO" name="Magnesium Oxide, Magnesia" status="" percent="0.510" tolerance=""/>
<oxide symbol="K2O" name="Potassium Oxide" status="" percent="0.670" tolerance=""/>
<oxide symbol="Na2O" name="Sodium Oxide, Soda" status="" percent="0.550" tolerance=""/>
<oxide symbol="P2O5" name="Phosphorus Pentoxide" status="" percent="0.090" tolerance=""/>
<oxide symbol="TiO2" name="Titanium Dioxide, Titania" status="" percent="0.530" tolerance=""/>
<oxide symbol="Al2O3" name="Aluminum Oxide, Alumina" status="" percent="20.480" tolerance=""/>
<oxide symbol="SiO2" name="Silicon Dioxide, Silica" status="" percent="66.210" tolerance=""/>
<oxide symbol="Fe2O3" name="Iron Oxide, Ferric Oxide" status="" percent="1.600" tolerance=""/>
<oxide symbol="MnO" name="Manganous Oxide" status="" percent="0.030" tolerance=""/>
</oxides>
<volatiles>
<volatile symbol="LOI" name="Loss on Ignition" percent="8.210" tolerance=""/>
<volatile symbol="SO3" name="Sulfur Trioxide" percent="0.090" tolerance=""/>
</volatiles>
</material>
Copyright 2003, 2008 http://digitalfire.com, All Rights Reserved
|
|
INSIGHT is ceramic chemistry
calculation software that runs on
Windows, Mac and Linux and talks
to this web site. ()
|